Mixing Procedure

Mixing procedure of Line Guard
(1) Shuzai and Kokazai of polymer cement emulsion are poured into a container.
(2) The paints are mixed with a stirrer for about three minutes.
(3) S Compound and C Compound are added little by little into the paint and mixed for about five minutes to get the uniform material.
Mixing Procedure of Pillar Coat
(1) Shuzai and Kokazai of polymer cement emulsion are poured into a container.
(2) The paints are mixed with a stirrer for about three minutes.
(3) S Compound is added little by little into the paint and mixed for about five minutes.

(Caution) In case of spraying, clear water is added for 1-1.5 litter for coordination of stickiness.



Test Results

Chart A: Test results of Pillar Coat
test itemsTest ResultsMethod of tests
basic characteristicsTest of permeating water with a pressure0.14According to JIS A-1404 (display of the ratio of permeated water)
Test of sucking water0.57According to JIS A-1404 (display of the ratio of sucked water)
Test of attachment power26kg/square cmsadhesive strength test by the Architecture Laboratory of the Minstry of Construstion
Test of strongness against bending28kg/square cmsAccording to JIS A-1404
Test of strongness against compression150kg/square cmsAccording to JIS A-1404
Test of strongness against abrasion1.5kg/500 timesTabor abrasion tester
Test of strongness against shock50cm/1000gDu-Pont impact tester
durabilityWater-proof test24kg/square cmsTest of attachment power by adhesive strength test by the Architecture Laboratory of the Minstry of Construction (permeated for two years)
Weather-proof test30kg/square cmsTest of attachment power by adhesive strength test by the Architecture Laboratory of the Minstry of Construction (exposed in outdoors for two years)
Weather-proof test for procedureMore than 9HHardness test of the pencil (weather-o-meter 1000hours)
Stability test for freezing and dissolution35kg/square cmsTest of attachment power by adhesive strength test by the Architecture Laboratory of the Minstry of Construction *1
Durability test against salty waterMore than 9HHardness test of the pencil (permeated for one month)
Durability test against salty waterMore than 9HHardness test of the pencil (permeated for one month)
Durability test against alkaliMore than 9HHardness test of the pencil (permeated for one month)
Durability test against acid3HHardness test of the pencil (permeated for one month)
*1 (40 degrees x 12 hours, 10 degrees x 12 hours) x 20 cycles

Chart B: Elution Tests of Line Guard
Name of the tested materialThe number of the testAnalyzed items
SnCdAsPbPCBHgCu
Line GuardK459not detected
<0.1
not detected
<0.002
not detected
<0.02
not detected
<0.01
not detected
<0.0005
not detected
<0.0005
0.08

Method of Line Guard measurement
SnJIS K 0102 63.1 Method of measuring briliantness
CdJIS K 0102 55.2 Method of measuring atomic briliantness
AsJIS K 0102 61.1 Method of measuring briliantness
PbJIS K 0102 54.2 Method of measuring atomic briliantness
PCBNotice No.59 by the Environment Agency gas chromatographic analysis rules
HgNotice No.59 by the Environment Agency Method of measuring atomic briliantness
CuJIS K 0102 52.2 Method of measuring atomic briliantness
*The unit is mg/l. The method of elution tests follow the Notice No.13 by the Environment Agency.